Titanium Crevice Corrosion: When Grade 2 Is Not Enough

Grade 2 titanium is immune to pitting in seawater. It is not immune to crevices. In a tight metal-to-metal gap at 80 °C (176 °F) in neutral chloride, the alloy that lasts twenty years in a condenser can groove a gasket face badly enough to leak within two.

The answer is Grade 7 or Grade 12 where the crevice has to stay, or a joint detail that removes it. The design route is much cheaper.

Inside the Gap

Titanium's oxide film needs water and oxygen to repair itself. Inside a crevice, oxygen is consumed faster than it diffuses in, so the gap becomes deaerated and its potential drops. Metal ions hydrolyse, local pH falls, chlorides migrate in to balance the charge, and the film stops reforming. Attack is then self-sustaining and fast: a 2 mm band can lose more metal in a year than the rest of the component loses in its life.

That makes crevice corrosion a temperature and geometry problem, not a chemistry problem alone. Bulk seawater at 30 °C rarely does it. The same water at 80 °C behind a gasket does. A deposit or scale creates the same conditions at lower bulk temperature, because the metal underneath runs hotter and starved of oxygen.

Alloys That Resist It

Palladium and molybdenum-nickel both work by making the passive film easier to reform in a deaerated acid gap. They are not interchangeable on cost or on strength.

GradeCompositionStrength (Rm min)Where it holdsWhen to choose it
Grade 2CP titanium345 MPaClean flowing seawater below about 70 °C, no tight gapsWhenever the crevice can be designed out
Grade 7Ti-0.2Pd, Pd 0.12–0.25%345 MPaHot chloride plus reducing acid; widest margin against crevice attackDilute HCl or H₂SO₄ service, hot and chlorinated
Grade 11Ti-0.2Pd in plate and strip345 MPaSame duty as Grade 7 in sheet formTank linings and vessel internals
Grade 12Ti-0.3Mo-0.8Ni483 MPaHot neutral brine, deposits, unavoidable crevicesWhen the medium is not strongly reducing and wall thickness matters

Grade 12 is the value choice in hot-brine work. It is alloyed with molybdenum and nickel rather than palladium, so its price does not track the precious-metal market, and its 483 MPa minimum allows a wall about 29% thinner than Grade 2 at the same design pressure. That buys back part of the premium on a vessel. Grade 7 still holds the wider envelope where the medium is genuinely reducing.

Two boundaries matter. In sour service, NACE MR0175 / ISO 15156 governs, and titanium grades appear only within stated limits on temperature, chloride and pH. Read the table, not the datasheet. Where fluoride is present, even at trace level in an acid stream, no titanium grade survives; it is the chemistry a pickling bath uses to dissolve titanium on purpose.

Where Crevices Hide

Most failures are not in the alloy selection. They are in a joint nobody thought of as a joint.

LocationWhy it is a creviceDesign fix
Lap or fillet weldUnwelded interface under the weld toe is a gap by constructionFull-penetration butt weld, root blended
Flange gasket faceFibrous gaskets wick and hold chloride against the facePTFE-filled spiral wound gasket, correct preload
Tube-to-tubesheet jointRoller expansion leaves a micro-gap behind the rollSeal weld after expansion
Support saddle or padMetal contact plus stagnation and a thermal bridgeRated non-metallic pad, or lift the pipe clear
Threaded connectionRoot of the thread is deaerated and cannot be cleanedWelded or flanged joint; sealant is not a fix
Deposit or scaleUnder-deposit environment mirrors a creviceKeep velocity above the settling threshold

Two Field Cases

A brine line at 90 °C with Grade 2 flanges failed at the gasket outside diameter, not in the pipe: a 1.5 mm deep groove in a 2 mm wide band, with the rest of the flange at nominal wall. Grade 12 flanges to the same dimensions lasted. The cheaper change, though, was the gasket and the face finish, which closed the wicking path.

A heat exchanger with Grade 2 tubes in 110 °C chloride showed wall loss only at the rolled joints. The tubes were fine. The joint was the component. Seal welding the tube ends cost less than retubing in Grade 7, and it removed the crevice rather than resisting it.

Finding It Early

Crevice attack is local by definition, so a spot reading on a clean shell misses it. Ultrasonic thickness mapping along known crevice lines (gasket bands, support contacts, weld toes) shows the signature as a narrow trough rather than general loss. A boroscope at the joint during a shutdown costs an hour and finds the problem while the answer is still a gasket and a weld prep.

For new work, Grade 7 and Grade 12 titanium bar covers flanges, fasteners and small forgings, and Grade 12 titanium plate covers vessels and linings. The grades chart sets mechanical minimums side by side. Duty notes sit on the chemical processing page and the marine and offshore page.

Medium and Joint Detail

Send the chloride level, the temperature, the pH and the joint drawing. We will quote Grade 2, 7 or 12 to the applicable ASTM specification and mark on the drawing where the crevice is, because moving one weld often beats upgrading the alloy.

Request a Corrosion Grade Review

CATEGORIES

CONTACT US

Contact: Jessie

Phone: +86-19539017809

E-mail: sales@gktitanium.com

Add: BLOCK A, HUIHANG PLAZA , HANGTUO ROAD, NATIONAL CIVIL AEROSPACE INDUSTRY BASE, Xi'an