Welcome: Shaanxi Guangke Titanium Industry Co., Ltd.

sales@gktitanium.com +86-19539017809

Industry news

Machining Titanium: Heat, Edges and Parameters

Machining titanium is a heat problem, which is why a metal softer than many steels at the same strength destroys edges faster. It carries heat away from the cut about seven times less effectively than steel. Heat, tool, coolant, rigidity and deflection explain most of the distance between a shop getting 40 parts per edge in Ti-6Al-4V and a shop getting 8.

Where the Heat Goes

Titanium conducts heat at roughly 7 W/m·K against about 50 W/m·K for steel. In a turning cut most of that heat stays at the tool edge and in the workpiece. The edge reaches temperatures where carbide softens, and the insert that survived 200 parts in 4140 fails at the twelfth part here.

So: low cutting speed, and a feed high enough to keep the edge under the chip instead of rubbing the surface. Carbide turning in Ti-6Al-4V runs at 30–60 m/min (100–200 sfm). At 80 m/min the edge looks fine for ten minutes, then fails suddenly. Titanium gives none of steel's gradual flank-wear warning.

Sharp, Dedicated Edges

Go with sharp positive-rake carbide in a dedicated titanium grade, usually uncoated or PVD-coated fine grain. Thick AlTiN or TiCN coatings that work well on steel tend to react with titanium and spall, and a worn coating is worse than no coating because the exposed substrate rubs.

Two habits cost more than they save: an insert that already ran on steel, where micro-chipping starts a crack, and a skipped finish pass, where a dull edge on 0.3 mm of stock ruins the next part's tolerance.

Coolant at the Edge

Flood coolant landing 20 mm from the contact point does very little for titanium. High-pressure through-tool coolant at 50–70 bar separates a stable cut from a fire risk, and it is the highest-return upgrade for a shop moving into titanium.

Without through-tool, aim the nozzle at the flank with the highest flow the pump will give. Never run titanium dry on a finishing pass. Never blow compressed air into a pocket holding titanium fines either; a chip fire is expensive in ways that never appear on the quote.

Rigidity First

A flexible setup turns a good parameter set into chatter, and chatter in titanium breaks edges in seconds. Keep tool overhang under three times the diameter, support the part under the cut rather than at its ends, and climb mill so the chip starts thick and thins out.

On thin walls, leave 0.5 mm (0.02 in) per side for a light final pass and re-check the wall after roughing. Titanium moves when the stressed layer comes off, and a part that was true in the blank can finish 0.1 mm out.

Tool Deflection

When the cutter is pushed off the line, feed per tooth collapses and the edge rubs. The symptom is a polished, work-hardened surface, a squealing cut and fast edge failure. The usual misdiagnosis is "bad material".

The fix is geometric: less radial engagement, shorter overhang, or the same material in two passes. Trochoidal milling, with small radial engagement at full depth and constant feed, is the standard answer in Ti-6Al-4V because it holds chip load steady and keeps the heat in the chip. Keep the tool moving as well. A 0.2 second dwell in the cut can take an edge.

Starting Parameters

OperationMaterialSpeed (m/min)FeedNote
Turning, carbideGrade 260–1200.15–0.30 mm/revDepth of cut 1–3 mm, keep the edge loaded
Turning, carbideTi-6Al-4V30–600.10–0.25 mm/revDepth of cut 1–3 mm, no dwell at the end of the pass
Milling, carbideTi-6Al-4V40–700.06–0.12 mm/toothRadial 8–12% of diameter, axial 1–3 mm
Drilling, carbideTi-6Al-4V12–250.05–0.10 mm/revPeck 1–2 × diameter, through-tool coolant
TappingTi-6Al-4V4–8—Form taps preferred, 65% thread height
Bandsaw, bimetalAll grades15–250.03–0.08 mm/toothFlood, light pressure, let the blade cut

Ranges for sharp carbide with good coolant, not a guarantee. Prove out on the first part and change one variable at a time.

Stock That Machines Easier

Peeled or ground bar instead of pickled removes alpha case and scale before the bar reaches your machine. Cut blanks beat 6 m bars, because a squared blank saves the saw operation, the handling and the remnant nobody can use. Annealed and stress-relieved stock pays on thin walls, where less movement after roughing means fewer re-cuts. For fasteners and fixtures, hex and flat bar to size arrives with the mill scale already gone.

Size and tolerance choices that reduce machining are collected in the size and tolerance guide. Our peeled and ground Grade 5 titanium bar and Grade 2 titanium bar ship on request, cut-to-size titanium plate usually removes a roughing operation entirely, and titanium hex and square bar covers the fastener stock.

Stock Size for the Cycle Time

Send the part drawing. We will propose the size, tolerance and condition that cut your machining time, and say when a near-net blank beats the material it wastes.

Request a Machining-Friendly Size

CATEGORIES

CONTACT US

Contact: Jessie

Phone: +86-19539017809

E-mail: sales@gktitanium.com

Add: BLOCK A, HUIHANG PLAZA , HANGTUO ROAD, NATIONAL CIVIL AEROSPACE INDUSTRY BASE, Xi'an